Fast Blister Repair with Six10

This repair method is tailored to fixing individual gelcoat blisters prior to bottom painting. The advantage of this method is it can repair blisters on hulls recently pulled from the water or hulls that have been out for some time. 

1. Open blisters with a small abrasive tool like 3M’s Rolock™
2" diameter sanding disk with 60-grit sandpaper. Make sure
you have removed the entire blister, including the edges of
the blister dome.

 

2. Wipe the cavity clean with an alcohol prep pad or
paper towels that have been soaked in isopropyl
alcohol. Be generous with the alcohol and change towels
frequently so the contaminants are removed rather than
spread. Repeat the alcohol wipe process and allow the
laminate to dry to the touch. It is particularly important to
repeat the alcohol-wipe on blisters that were fluid filled at
the time they were ground away.


3. Fill the cavities with Six10 Thickened Epoxy Adhesive
dispensed through the static mixing wand.

 

4. Spread the Six10 Adhesive flush with the surrounding
hull with a wide putty knife or plastic spreader. Avoid
overfilling the cavities because Six10 is difficult to sand.

 

5. Wet sand with 80–120-grit wet/dry sandpaper or wash
with water (no soap, no ammonia) and sand dull with
100-grit sandpaper. If you are using Six10 in warm
conditions, you should be able to wet sand and bottom
paint later the same day. If working in cooler temperatures,
allow the  epoxy to cure overnight before sanding.

6. Apply your bottom paint of choice. 

Why this method works 

Six10 Adhesive is epoxy thickened with fumed silica, which allows the epoxy to remain an excellent moisture barrier. When the static mixer is used to dispense it the blister cavity&nbspis filled with air free epoxy. This is important because small bubbles in coatings and putties degrade moisture barrier potential by creating short cuts for moisture to permeate the hull. In the end, Six10 produces a moisture barrier that is better than the original gelcoat. 

In our Gelcoat Blister manual, we recommend filling and fairing extensively blistered hulls with WEST SYSTEM® Epoxy thickened with one of our low-density fillers (407 Low Density or 410 Microlight®). The hollow microscopic spheres used to make low-density fillers easy to sand, make them poor moisture barriers. So, the blister manual requires that an effective epoxy barrier coat be applied over the filled and faired surface. 

Six10 Adhesive is an excellent option for filling ground out blister cavities—especially if you don’t plan to barrier coat to your hull. More good reasons for using Six10. Six10 is simple to use. No stirring is required when the epoxy is dispensed through the static mixer. The Six10 cartridge fits any standard caulking gun and always dispenses epoxy at the perfect mix ratio. Six10 makes filling blisters easy and efficient. This is comforting to know whether doing the job yourself or paying someone else to do it.  

More good reasons for using Six10.

Six10 is simple to use. No stirring is required when the epoxy is dispensed through the static mixer. The Six10 cartridge fits any standard caulking gun and always dispenses epoxy at the perfect mix ratio. Six10 makes filling blisters easy and efficient. This is comforting to know whether doing the job yourself or paying someone else to do it.

 

 

Epoxyworks - View our Epoxy Magazine Online SCFB       facebook    twitter   YouTube

WEST SYSTEM is a registered trademark of West System Inc | Sitemap | Terms & Conditions | Web Site by Ingenex Digital

Customers in Europe, Africa and the Middle East may be best served by West System International