Material
|
G/flex
|
Surface Prep/Conditions |
Tensile Adhesion (psi) |
| G-10 high-density laminate |
650 |
80-grit sand / dry surface
|
3459 |
| G-10 high-density laminate |
655 |
80-grit sand / wet surface |
2473 |
| 1018 steel |
650 |
80-grit sand / dry surface |
1772 |
| 1018 steel |
655 |
80-grit sand / wet surface |
3562 |
| Galvanized steel |
650 |
100-grit wet sand |
2562 |
| Galvanized steel |
655 |
100-grit wet sand |
2929 |
| Aluminum 2024 T3 |
650 |
80-grit sand, 860 etch / dry surface |
2731 |
| Aluminum 2024 T3 |
650 |
Grit blast, 860 etch / dry surface |
1856 |
| Aluminum 2024 T3 |
655 |
80-grit sand, 860 etch / wet surface |
1503 |
| Aluminum 2024 T3 |
655 |
80-grit sand, 860 etch / dry surface |
2153 |
| Copper |
650 |
80-grit sand |
2334 |
| Copper |
655 |
80-grit sand |
2685 |
| Bronze |
650 |
80-grit sand |
2782 |
| Bronze |
650 |
Scotch Brite™ pad sand |
2962 |
| Bronze |
655 |
80-grit sand |
2936 |
| ABS plastic |
655 |
80-grit sand |
1535 |
| ABS plastic |
655 |
80-grit sand, flame treat |
1813 |
| ABS plastic |
655 |
Alcohol wipe, flame treat |
3288 |
| PVC |
655 |
80-grit sand |
1780 |
| PVC |
655 |
80-grit sand, flame treat |
1813 |
| PVC |
655 |
Alcohol wipe, flame treat |
2081 |
| Polyethylene (HDPE) |
655 |
80-grit sand |
400 |
| Polyethylene (HDPE) |
655 |
80-grit sand, flame treat |
1890 |
| Polyethylene (HDPE) |
655 |
Alcohol wipe, flame treat |
2312 |
| Polycarbonate (Lexan®) |
655 |
80-grit sand |
1870 |
| Ipe |
650 |
60-grit sand |
2134 |
| Ipe |
655 |
Plane, isopropyl alcohol wipe x 3 |
2223 |
| Teak, vertical grain |
650 |
80-grit sand parallel to grain
|
1413 |
| Teak, vertical grain |
655 |
80-grit sand parallel to grain |
1381 |
| Teak, vertical grain |
655 |
80-grit sand, alcohol wipe x 2
|
1503 |
| White oak, vertical grain |
650 |
80-grit sand |
1935 |
| White oak, vertical grain |
655 |
80-grit sand |
1780 |
| White oak, vertical grain |
655 |
Alcohol wipe x 2 |
2212 |
| Purpleheart |
650 |
60-grit sand parallel to grain |
1731 |